1/4" phenolic sheet 
 5-Layer Fiberglass10-Layer Fiberglass
Control (West Systems epoxy)  
West Systems + Phenolic microballoons  
West Systems + Cork microballoons  
West Systems + High temperature paint  
West Systems + Cotronics 4700  

Fiberglass Sample Preparation:

  1. Used West Systems epoxy to make 4 of 8" x 8" sheets of fiberglass (2 x 5 layers, 2 x 10 layers), making sure to put Mylar beneath to keep the samples from sticking. 
  2. Let the samples cure for at least 24 hours. 
  3. Sanded with a Dremel, then with 400-grit sandpaper. Make sure to sand the shiny side as well
  4. Mark and cut into 1.5" x 1.5" squares.
  5. Recorded dry mass of each sample (series 1-9)
  6. Took three measurements of thickness on three different sides, and calculated/recorded average thickness (series 1-9)
  7. Wearing respirators, mixed 50 g. West Systems resin + 9 g West Systems hardener (100:18 ratio for West Systems, but this depends on the epoxy you choose to use)
  8. Mixed in phenolic microballoons using a popsicle stick until a consistency slightly thinner than peanut butter (like melted ice cream) was reached.
  9. Applied an even but thin layer of phenolic mixture to samples (series 4, 5, 8, 9) using popsicle sticks
  10. Let samples and left to cure for 36 hours.
  11. Recorded average thickness of samples with phenolic coating (series 4, 5, 8, 9)
  12. Sanded with 400-grit sandpaper then recorded mass (and wiped with acetone)
  13. Applied high-temp paint to fiberglass samples (series 6,7) and fiberglass + phenolic samples (series 8,9)
  14. Let paint dry for at least 24 hours (depending on what paint you use)
  15. Record mass of each sample (series 6, 7, 8, 9)
  16. Record average thickness of each sample (series 6, 7, 8, 9)

Below is the test matrix for the parameters measured during this test. (MAKE SUMMARY, ATTACH EXCEL FILE).

...