  1. We cut out many rectangles of fiberglass, in several sizes. We probably cut approximately 30 each of 3"x4", 4"x8", and 10"x12", as well as 6 strips of 3"x48".
  2. We laid out the mold halves next to each other, mold side up and pointing the same way.
  3. We coated the mold halves in many, many layers of mold release.
  4. We coated the nose cone part of the mold with gelcoat to provide a better surface finish. We did not have enough remaining gelcoat for the coupler section, but the mylar provided a superior surface finish.
  5. We placed a strip on the right side of each mold, and wetted it with epoxy.
  6. We placed a strip of wax paper on the left side of each mold, covering about 1-2" of the mold surface.
  7. We placed fiberglass rectangles on the mold, and squeegeed epoxy onto the fabric.
  8. We repeated step 2 until we had completed 5 layers near the tip, 7 layers near the base and 9 layers in the coupler.
  9. We folded over the glass on the left side of the mold to make space, and removed the wax paper.
  10. We put together the mold halves, taking care to insert the free fiberglass strip under the folded-over fiberglass so that they overlapped. A useful trick here was to use scrap aluminum as a shim, to keep the mold halves apart while we reached our hands into the parting line.
  11. We used the stick (accessory tool pictured above) to fold back the folded-over fiberglass, such that the layers overlapped.
  12. We used the stick to apply 4 more strips of fabric on the inside of the nosecone; 2 on either side.
  13. We moved the nosecone to the floor, with the cone pointing downwards.
  14. We used two very large clamps to clamp together the coupler section, and some weights to push the rest of the mold together.
  15. We used two balloons to apply pressure to the composite as it cured; the balloons were inflated with the vacuum pump because we were all wearing respirators.
  16. We left the part to cure overnight, and then removed it.

...

  • Large divots near the parting line: because the cavity was so large, it was very difficult to make the overlap neat, so some areas didn't overlap correctly.
  • Stray tufts of fiberglass inside the nosecone: because we weren't able to reach the end of the nosecone, the tip of the nosecone was blocked off by stray tufts of fiberglass that weren't smoothed out.

In the future, there are a few things we would like to change:

  • Since the coupler did not need to sanded in order to fit inside the tubes, a 7-ply coupler should be plenty.
  • The number of plies should be decreased after we complete our structural testing