Manufacturing Procedure:

  • Wet sand mold to 2000 grit using sanding block (made of foam)
  • Wax mold (3 layers of Mold Release Wax, yellow container)
  • Apply PVA film with fine-haired brush, let set for 20 minutes
  • Mix cabosil + epoxy and apply to mold (thick on edges)
  • Layup- don't wet plies before laying down
  • Tab at least 1" at base, shorter at tip
  • Vacuum bag
  • Mold release: use chiseled popsicle sticks and hammer (add more until pops open)
  • Apply ablative (using layup jig)
  • Use heat gun to dry (don't overwork)
  • Oven cure
  • Sand outside
  • Sand inside (seam)
  • Plane ends
  • Fill low spots with ablative + epoxy mixture
  • Paint

 

Lessons Learned:

  • Don't coat the mold multiple times with epoxy - just once, let soak and WIPE, then cure and sand
  • Protect edges with aluminum or something rigid and straight to prevent them from getting rounded
  • Do not wipe mold with acetone once PVA film has been applied or it will come off

 

 

  • No labels